Flat glass sheet: Bill of materials
About these figures
Which unit, study and year the composition figures describe, and how they vary
Clear float inputs are calculated: Guardian's batch shares [11] applied to 9.2 kg of raw materials for 10 kg of glass at 20% cullet, using the 1.18 to 1.22 kg of raw material that 1 kg of cullet replaces [9]; about 2.3 kg of the batch is cullet, a recycled input with no node. Solar inputs use per-tonne figures from a 2025 PV glass review, applied to 8 kg per m2. Inputs are not shares of the glass, so mass shares are left empty. Salt cake, carbon and iron oxide are small and not linked. Mass per mm is from AGC and Saint-Gobain EPDs [1, 5].
as of 2026-11-13
Direct materials
The commodities and chemicals in one unit as bought, with amount, mass share, cost share and recycled content
Variant 1 Clear float| Material | Role | Amount in one unit | Share of the unit's mass |
|---|---|---|---|
| Qz Silica sand | Structural | 6.69 kgrange 5.93 to 7.53 kg | – |
| Silica sand, approximately 70 to 75% of the batch by weight [11]; calculated: the Guardian shares are of the raw-material batch, applied to the raw materials for 10 kg of glass, 9.23 kg at 20% cullet (low 8.47 kg at 25% cullet, high 10.04 kg at 15%), taking 1.18 to 1.22 kg of raw material per kg of glass from the cullet ratio in [9] | |||
| Sda Soda ash | Functional | 1.38 kgrange 1.27 to 1.51 kg | – |
| Soda ash, 15% of the batch [11], lowers the melting temperature; calculated: the Guardian shares are of the raw-material batch, applied to the raw materials for 10 kg of glass, 9.23 kg at 20% cullet (low 8.47 kg at 25% cullet, high 10.04 kg at 15%), taking 1.18 to 1.22 kg of raw material per kg of glass from the cullet ratio in [9] | |||
| Stn Crushed stone | Functional | 1.38 kgrange 1.27 to 1.51 kg | – |
| Limestone and dolomite, 15% of the batch together [11], linked to crushed stone (raw limestone, not burnt lime); calculated: the Guardian shares are of the raw-material batch, applied to the raw materials for 10 kg of glass, 9.23 kg at 20% cullet (low 8.47 kg at 25% cullet, high 10.04 kg at 15%), taking 1.18 to 1.22 kg of raw material per kg of glass from the cullet ratio in [9] | |||
| Material | Role | Amount in one unit | Share of the unit's mass |
|---|---|---|---|
| Qz Silica sand | Structural | 5.96 kgrange up to 6.4 kg | – |
| Low-iron quartz sand, 745 kg per tonne of PV glass in one source and 800 kg in another, applied to 8 kg per m2 at 3.2 mm (calculated) [9] | |||
| Sda Soda ash | Functional | 2.03 kgrange 1.04 to 2.03 kg | – |
| Soda ash, 254 kg per tonne of PV glass in one source and 130 kg in another, applied to 8 kg per m2 (calculated; low uses 130 kg) [9] | |||
as of 2026-11-13
Cost breakdown
The share of the unit's cost in each component or stage
| Part | Share of cost | Variant | Year | Source |
|---|---|---|---|---|
| Raw materials | 48% | Low-iron solar | 2025 | [9] |
as of 2026-11-13
How it is put together
The main steps from parts and materials to the finished unit
| Step | What happens | Technology | Source |
|---|---|---|---|
| Batch preparation | Sand, soda ash, limestone and dolomite are weighed and mixed; 15 to 25% of the batch is crushed recycled glass [11] | – | [11] |
| Melting | The batch melts in a gas-fired furnace with a melting zone of about 1,500 to 1,600 degrees Celsius [11] | Glassmaking | [11] |
| Floating | The glass pours continuously on a bath of molten tin and spreads into a ribbon of 2 to 19 mm [11] | Float glass | [11] |
| Cooling | The ribbon is cooled gradually in a temperature-controlled lehr so that it can be cut [11] | – | [11] |
| Cutting and inspection | The ribbon is cut into stock sheets, and cameras or laser sensors detect defects [11] | – | [11] |
as of 2026-11-13
Technologies used to make it
The technologies used to make it, at which step
Made with- Gl Glassmaking Melting the batch Soda-lime glassmaking is the melting step; no share figure is given.
- FG Float glass Forming the ribbon on molten tin Float forming makes clear glass; most PV front glass is rolled instead (95%) [9]
as of 2026-11-13
Sources
- Low-Carbon Planibel Clearlite 4 mm (EPD) AGC Glass Europe, EPD verified under the FDES INIES programme (HQE Association), 2024
- PARSOL flat glass from 3 mm to 10 mm, body tinted glass (Environmental Product Declaration) Saint-Gobain Glass Industry, Europe; The International EPD System, 2021
- Review of issues and opportunities for glass supply for photovoltaic production at multiterawatt (TW) scale Sustainable Energy and Fuels (Royal Society of Chemistry); T. Chowdhury, M. Dehghanimadvar, N.L. Chang and R. Corkish, 2025
- A short guide to how glass is made Guardian Glass