Per tonne of finished sheet. Silicon is about 3.2% of thyssenkrupp's hot-rolled base strip (2021 production) [4] and about 3% in a general source, which adds about 96.5% iron and 0.5% other elements [9]. The EPD records 127 kg of secondary material per tonne [4]. Inhibitor elements such as manganese and aluminium, and the coating, are small amounts that no opened source quantifies, so they are not counted. Cores, laminations and non-oriented steel are not yet nodes.
as of 2026-11-15
Direct materials
The commodities and chemicals in one unit as bought, with amount, mass share, cost share and recycled content
| Material | Role | Amount in one unit | Share of the unit's mass | Recycled content |
|---|---|---|---|---|
| Fe Iron ore | Structural | 965 kg | 96.5% | 12.7% |
| About 96.5% iron [9]; the EPD records 127 kg of secondary material per tonne, calculated as 12.7% [4]. Iron comes from ore and from scrap. Iron ore is the nearest node, so the amount is iron content, not ore mass. | ||||
| Si Silicon | Functional | 32 kgrange 30 to 33 kg | 3.2% | – |
| Silicon is about 3.2% of the base strip [4] (32 kg per tonne, calculated), about 3% in a general source [9], and normally below 3.30% [7]. It is added as silicon alloys [1]. | ||||
as of 2026-11-15
How it is put together
The main steps from parts and materials to the finished unit
| Step | What happens | Technology | Source |
|---|---|---|---|
| Melt and cast | Steel scrap and silicon alloys are melted and cast into slabs. | – | [1] |
| Reheat and hot roll | Slabs are reheated to dissolve the inhibitor compounds, then hot rolled to heavy coils; hot rolling loses 3.5% of the metal. | – | [1] |
| Cold roll | The coil is cold rolled to final thickness; this step loses under 0.025% of the metal. | – | [1] |
| High-temperature anneal | Coils are held above 1,100 C for more than 10 hours; the steel is purified, the aligned crystals grow and a forsterite film forms. The whole cycle takes 4 to 6 days. | – | [17] |
| Coat and refine domains | The coil is trimmed again, annealed, laser treated to develop the grain orientation and coated; the best grades have their domains refined by laser. | Laser | [1][8] |
| Cut and stack | Transformer makers cut the sheet into laminations and stack them into the core. | – | [1] |
as of 2026-11-15
Technologies used to make it
The technologies used to make it, at which step
Made with- Lsr Laser Laser irradiation of the sheet surface to refine magnetic domains (domain-refined grades) One maker's HI-B LS grade is made this way [8]; no share of output found.
as of 2026-11-15
Sources
- Electric Grid Supply Chain Review: Large Power Transformers and High Voltage Direct Current Systems US Department of Energy, 2022
- Environmental Product Declaration EPD-TKE-20240546-CBC1-EN: powercore grain oriented electrical steel thyssenkrupp Electrical Steel, programme holder Institut Bauen und Umwelt e.V. (IBU), 2025
- The processing, microstructure, texture, and magnetic properties of electrical steels: A review (He and Kestens, International Materials Reviews 70(5), 353-393) TU Delft repository copy, 2025
- Grain-Oriented Electrical Steel Sheets (ORIENTCORE product page) Nippon Steel Corporation, 2026
- Electrical steels Megger (Electrical Times online), 2010